无机材料学报 ›› 2016, Vol. 31 ›› Issue (12): 1347-1354.DOI: 10.15541/jim20160146 CSTR: 32189.14.10.15541/jim20160146

• • 上一篇    下一篇

氧化还原沉淀法制备MnO2/MWCNTs催化剂及其低温SCR活性

陈 健, 郑玉婴, 张延兵, 邹海强, 卢秀恋   

  1. (福州大学 材料科学与工程学院, 福州 350108)
  • 收稿日期:2016-03-15 修回日期:2016-04-25 出版日期:2016-12-16 网络出版日期:2016-11-23
  • 基金资助:
    基金项目: 福州市科技计划(2015H0016) Science and Technology Program of Fuzhou (2015H0016)

Preparation of MnO2/MWCNTs Catalysts by a Redox Method and Their Activity in Low-temperature SCR

CHEN Jian, ZHENG Yu-Ying, ZHANG Yan-Bing, ZOU Hai-Qiang, LU Xiu-Lian   

  1. (College of Materials Science and Engineering, Fuzhou University, Fuzhou 350108, China)
  • Received:2016-03-15 Revised:2016-04-25 Published:2016-12-16 Online:2016-11-23

摘要:

先用十二烷基硫酸钠(SDS)对多壁碳纳米管(MWCNTs)进行表面改性, 然后采用氧化还原沉淀法制得一系列的MnO2/MWCNTs催化剂。考察了催化剂在80~180℃的选择性催化还原(SCR)反应活性, 并通过BET、XRD、FESEM、TEM、XPS和H2-TPR等表征手段对催化剂的结构及性能进行分析。结果显示, MnO2/MWCNTs催化剂在空速210 L/(gcat·h)和温度140~180℃条件下, 脱硝效率达到85%~100%, 这明显优于等体积浸渍法制备的催化剂的低温SCR催化活性, 且10% MnO2/MWCNTs催化剂的活性最优。分析结果表明, MnO2/MWCNTs催化剂中MnO2以纳米片状均匀分散在多壁碳纳米管载体表面; 弱结晶性的结构和高价锰, 较高的表面吸附含氧量及较强的低温区氧化还原能力是10% MnO2/MWCNTs催化剂具有优异低温SCR活性的原因。另外, 和MnOx/MWCNTs催化剂相比, 10% MnO2/MWCNTs催化剂表现出良好的抗水和抗硫性能。

关键词: 十二烷基硫酸钠, 选择性催化还原, 氮氧化物, 多壁碳纳米管, 锰氧化物

Abstract:

Pristine multiwalled carbon nanotubes (MWCNTs) were modified by sodium dodecyl sulfate (SDS). Afterwards, a series of MnO2/MWCNTs were prepared via a redox method and used in selective catalytic reduction (SCR) of NOx at 80-180℃. Structural properties and catalytic performance were investigated by specific surface area measurements (BET), X-ray diffraction (XRD), filed emission scanning electron microscope (FESEM), transmission electron microscope (TEM), X-ray photoelectron spectroscope (XPS), and H2 temperature-programmed reduction (H2-TPR). The characterization results indicate that the nanoflaky MnO2 highly disperse on MWCNTs. The results show that the low-temperature SCR activities of MnO2/MWCNTs catalysts are 85%-100% at 140-180℃ at a weight hourly space velocity of 210 L/(gcat·h), higher than that of catalyst fabricated via the wet impregnation method. The 10% MnO2/MWCNTs catalyst displays first-rate SCR activity, which is attributed to its low crystallinity, high concentrations of Mn4+ and oxygen absorbtion onto the catalyst surface, as well as excellent reducibility. Additionally, compared to the MnOx/MWCNTs catalyst, the 10% MnO2/MWCNTs catalyst exhibits higher resistance to H2O and SO2.

Key words: sodium dodecyl sulfate, selective catalytic reduction, nitrogen oxide, multi-walled carbon nanotube, manganese oxide

中图分类号: