Journal of Inorganic Materials ›› 2026, Vol. 41 ›› Issue (11): 1677-1685.DOI: 10.15541/jim20260078
• RESEARCH ARTICLE • Previous Articles Next Articles
XU Jiawei1,2(
), LI Xiang1, ZHANG Jing1,2, XIE Jiansheng1, DENG Mingxue1,2, QI Xuejun1, CHEN Junfeng1,2(
)
Received:2026-02-24
Revised:2026-04-21
Published:2026-05-19
Online:2026-05-19
Contact:
CHEN Junfeng, professor. E-mail: jfchen@mail.sic.ac.cnAbout author:XU Jiawei (2001-), male, Master candidate. E-mail: xujiawei22@mails.ucas.ac.cn
Supported by:CLC Number:
XU Jiawei, LI Xiang, ZHANG Jing, XIE Jiansheng, DENG Mingxue, QI Xuejun, CHEN Junfeng. Gamma-ray Induced Radiation Damage in BaF2:Y Scintillation Crystals[J]. Journal of Inorganic Materials, 2026, 41(11): 1677-1685.
Fig. 2 Optical transmittance spectra of Y0-Y20 samples before irradiation (black solid lines) and after 10 Mrad irradiation (blue solid lines), and normalized RL spectra (red dashed lines) Colorful figure is available on website
Fig. 3 RIAC spectra (black solid lines), individual fitted peaks (blue dashed lines), and total fitted curves (red solid lines) of Y0-Y20 samples after 10 Mrad irradiation Colorful figures are available on website
| Sample | Peak | ||||||
|---|---|---|---|---|---|---|---|
| a/a′ | b | c/c′ | d | e | f/f′ | ||
| Y0 | Position/eV | 1.59 | 2.15 | 2.79 | 4.03 | 5.05 | 5.96 |
| Y1 | 1.76 | - | 2.82 | 4.06 | 5.01 | 6.35 | |
| Y2 | 1.79 | - | 2.82 | 4.02 | 5.04 | 6.54 | |
| Y5 | 1.88 | - | 2.84 | 3.98 | 5.00 | 6.46 | |
| Y7.5 | 1.89 | - | 2.88 | 3.99 | 5.17 | 6.55 | |
| Y10 | 1.91 | - | 2.93 | 4.02 | 5.06 | 6.50 | |
| Y15 | 1.93 | - | 2.93 | 4.00 | 5.16 | 6.53 | |
| Y20 | 1.95 | - | 2.97 | 4.00 | 5.13 | 6.59 | |
| Y0 | FWHM/eV | 0.47 | 0.64 | 1.13 | 1.05 | 0.93 | 1.32 |
| Y1 | 0.36 | - | 1.18 | 1.00 | 1.28 | 1.25 | |
| Y2 | 0.43 | - | 1.15 | 1.03 | 1.52 | 1.21 | |
| Y5 | 0.48 | - | 0.94 | 1.17 | 1.08 | 1.27 | |
| Y7.5 | 0.36 | - | 0.85 | 1.27 | 1.42 | 1.16 | |
| Y10 | 0.37 | - | 1.00 | 1.10 | 1.21 | 1.36 | |
| Y15 | 0.36 | - | 1.00 | 1.24 | 1.40 | 1.33 | |
| Y20 | 0.35 | - | 0.98 | 1.14 | 1.52 | 1.38 | |
Table 1 Peak positions and their FWHMs of radiation-induced absorption spectra for Y0-Y20 samples after 10 Mrad irradiation
| Sample | Peak | ||||||
|---|---|---|---|---|---|---|---|
| a/a′ | b | c/c′ | d | e | f/f′ | ||
| Y0 | Position/eV | 1.59 | 2.15 | 2.79 | 4.03 | 5.05 | 5.96 |
| Y1 | 1.76 | - | 2.82 | 4.06 | 5.01 | 6.35 | |
| Y2 | 1.79 | - | 2.82 | 4.02 | 5.04 | 6.54 | |
| Y5 | 1.88 | - | 2.84 | 3.98 | 5.00 | 6.46 | |
| Y7.5 | 1.89 | - | 2.88 | 3.99 | 5.17 | 6.55 | |
| Y10 | 1.91 | - | 2.93 | 4.02 | 5.06 | 6.50 | |
| Y15 | 1.93 | - | 2.93 | 4.00 | 5.16 | 6.53 | |
| Y20 | 1.95 | - | 2.97 | 4.00 | 5.13 | 6.59 | |
| Y0 | FWHM/eV | 0.47 | 0.64 | 1.13 | 1.05 | 0.93 | 1.32 |
| Y1 | 0.36 | - | 1.18 | 1.00 | 1.28 | 1.25 | |
| Y2 | 0.43 | - | 1.15 | 1.03 | 1.52 | 1.21 | |
| Y5 | 0.48 | - | 0.94 | 1.17 | 1.08 | 1.27 | |
| Y7.5 | 0.36 | - | 0.85 | 1.27 | 1.42 | 1.16 | |
| Y10 | 0.37 | - | 1.00 | 1.10 | 1.21 | 1.36 | |
| Y15 | 0.36 | - | 1.00 | 1.24 | 1.40 | 1.33 | |
| Y20 | 0.35 | - | 0.98 | 1.14 | 1.52 | 1.38 | |
| Sample | EWRIAC/m-1 | ||||
|---|---|---|---|---|---|
| After 10 krad | After 100 krad | After 1 Mrad | After 10 Mrad | ||
| Y0 | Fast | 6.2 | 7.9 | 10.3 | 9.5 |
| Y1 | 2.6 | 4.6 | 5.2 | 5.5 | |
| Y2 | 2.1 | 2.9 | 4.5 | 4.6 | |
| Y5 | 3.4 | 4.3 | 6.2 | 9.5 | |
| Y7.5 | 5.1 | 7.0 | 8.8 | 9.3 | |
| Y10 | 4.6 | 8.9 | 13.4 | 12.7 | |
| Y15 | 8.8 | 15.2 | 22.2 | 23.8 | |
| Y20 | 9.2 | 18.1 | 25.9 | 29.7 | |
| Y0 | Slow | 4.2 | 6.6 | 8.7 | 8.4 |
| Y1 | 1.6 | 3.2 | 4.8 | 4.9 | |
| Y2 | 1.5 | 2.5 | 3.9 | 4.0 | |
| Y5 | 2.3 | 3.7 | 5.6 | 7.0 | |
| Y7.5 | 2.5 | 4.2 | 6.4 | 6.4 | |
| Y10 | 2.9 | 6.3 | 10.5 | 10.1 | |
| Y15 | 5.2 | 10.7 | 17.3 | 18.4 | |
| Y20 | 5.7 | 12.0 | 20.2 | 22.4 | |
Table 2 EWRIACs of the fast and slow components in Y0-Y20 samples after 10 krad to 10 Mrad irradiation doses
| Sample | EWRIAC/m-1 | ||||
|---|---|---|---|---|---|
| After 10 krad | After 100 krad | After 1 Mrad | After 10 Mrad | ||
| Y0 | Fast | 6.2 | 7.9 | 10.3 | 9.5 |
| Y1 | 2.6 | 4.6 | 5.2 | 5.5 | |
| Y2 | 2.1 | 2.9 | 4.5 | 4.6 | |
| Y5 | 3.4 | 4.3 | 6.2 | 9.5 | |
| Y7.5 | 5.1 | 7.0 | 8.8 | 9.3 | |
| Y10 | 4.6 | 8.9 | 13.4 | 12.7 | |
| Y15 | 8.8 | 15.2 | 22.2 | 23.8 | |
| Y20 | 9.2 | 18.1 | 25.9 | 29.7 | |
| Y0 | Slow | 4.2 | 6.6 | 8.7 | 8.4 |
| Y1 | 1.6 | 3.2 | 4.8 | 4.9 | |
| Y2 | 1.5 | 2.5 | 3.9 | 4.0 | |
| Y5 | 2.3 | 3.7 | 5.6 | 7.0 | |
| Y7.5 | 2.5 | 4.2 | 6.4 | 6.4 | |
| Y10 | 2.9 | 6.3 | 10.5 | 10.1 | |
| Y15 | 5.2 | 10.7 | 17.3 | 18.4 | |
| Y20 | 5.7 | 12.0 | 20.2 | 22.4 | |
Fig. 6 Normalized phosphorescence emission spectra (black solid lines), individual fitted peaks (blue dashed lines), and total fitted curves (red solid lines) of Y0-Y20 samples after 10 Mrad irradiation Colorful figures are available on website
| Sample | Peak | ||||||||
|---|---|---|---|---|---|---|---|---|---|
| A | B | C | D | E | F | G | H | ||
| Y0 | Position/eV | - | - | 2.30 | - | 2.85 | - | 3.25 | 3.73 |
| Y1 | 2.02 | 2.15 | 2.27 | 2.57 | 2.97 | 3.06 | 3.27 | 3.78 | |
| Y2 | 2.06 | 2.14 | 2.28 | 2.57 | 2.92 | 3.01 | 3.28 | 3.63 | |
| Y5 | 2.07 | 2.13 | 2.28 | 2.56 | 2.85 | 3.00 | 3.27 | 3.54 | |
| Y7.5 | 2.00 | 2.11 | 2.28 | 2.55 | 2.84 | 3.00 | 3.27 | 3.52 | |
| Y10 | 2.02 | 2.12 | 2.28 | 2.55 | 2.84 | 3.00 | 3.27 | 3.53 | |
| Y15 | 2.00 | 2.11 | 2.27 | 2.54 | 2.84 | 3.00 | 3.27 | 3.48 | |
| Y20 | 2.01 | 2.12 | 2.27 | 2.55 | 2.85 | 3.00 | 3.27 | 3.48 | |
| Y0 | FWHM/eV | - | - | 0.65 | - | 0.16 | - | 0.12 | 1.03 |
| Y1 | 0.08 | 0.08 | 0.06 | 0.09 | 0.08 | 0.06 | 0.20 | 1.70 | |
| Y2 | 0.28 | 0.08 | 0.06 | 0.11 | 0.15 | 0.09 | 0.27 | 1.63 | |
| Y5 | 0.25 | 0.06 | 0.06 | 0.11 | 0.07 | 0.10 | 0.17 | 1.41 | |
| Y7.5 | 0.07 | 0.08 | 0.06 | 0.10 | 0.08 | 0.11 | 0.14 | 1.38 | |
| Y10 | 0.14 | 0.09 | 0.07 | 0.11 | 0.07 | 0.11 | 0.14 | 1.32 | |
| Y15 | 0.08 | 0.08 | 0.07 | 0.11 | 0.09 | 0.11 | 0.14 | 1.32 | |
| Y20 | 0.10 | 0.08 | 0.07 | 0.11 | 0.07 | 0.10 | 0.15 | 1.34 | |
| Y0 | Fraction/% | - | - | 0.6 | - | 1 | - | 1.8 | 96.5 |
| Y1 | 0.1 | 0.7 | 0.2 | 0.7 | 0.1 | 0.1 | 2 | 96.1 | |
| Y2 | 0.7 | 0.9 | 0.5 | 1.7 | 0.4 | 0.7 | 6 | 89.1 | |
| Y5 | 1.5 | 0.5 | 1.3 | 1.9 | 0.2 | 1.3 | 4.8 | 88.4 | |
| Y7.5 | 0.8 | 1.4 | 3.3 | 2 | 0.9 | 3.4 | 8.8 | 79.3 | |
| Y10 | 1.6 | 1.3 | 2.7 | 2.7 | 0.3 | 1.5 | 5.1 | 84.8 | |
| Y15 | 2.5 | 4.4 | 10.2 | 6.4 | 0.9 | 3.3 | 8.7 | 63.6 | |
| Y20 | 2.9 | 4 | 8.9 | 5.5 | 0.4 | 2.3 | 7.3 | 68.7 | |
Table 4 Peak positions, FWHMs and relative integrated intensities (fractions) of the phosphorescence emission peaks in Y0-Y20 samples after 10 Mrad irradiation
| Sample | Peak | ||||||||
|---|---|---|---|---|---|---|---|---|---|
| A | B | C | D | E | F | G | H | ||
| Y0 | Position/eV | - | - | 2.30 | - | 2.85 | - | 3.25 | 3.73 |
| Y1 | 2.02 | 2.15 | 2.27 | 2.57 | 2.97 | 3.06 | 3.27 | 3.78 | |
| Y2 | 2.06 | 2.14 | 2.28 | 2.57 | 2.92 | 3.01 | 3.28 | 3.63 | |
| Y5 | 2.07 | 2.13 | 2.28 | 2.56 | 2.85 | 3.00 | 3.27 | 3.54 | |
| Y7.5 | 2.00 | 2.11 | 2.28 | 2.55 | 2.84 | 3.00 | 3.27 | 3.52 | |
| Y10 | 2.02 | 2.12 | 2.28 | 2.55 | 2.84 | 3.00 | 3.27 | 3.53 | |
| Y15 | 2.00 | 2.11 | 2.27 | 2.54 | 2.84 | 3.00 | 3.27 | 3.48 | |
| Y20 | 2.01 | 2.12 | 2.27 | 2.55 | 2.85 | 3.00 | 3.27 | 3.48 | |
| Y0 | FWHM/eV | - | - | 0.65 | - | 0.16 | - | 0.12 | 1.03 |
| Y1 | 0.08 | 0.08 | 0.06 | 0.09 | 0.08 | 0.06 | 0.20 | 1.70 | |
| Y2 | 0.28 | 0.08 | 0.06 | 0.11 | 0.15 | 0.09 | 0.27 | 1.63 | |
| Y5 | 0.25 | 0.06 | 0.06 | 0.11 | 0.07 | 0.10 | 0.17 | 1.41 | |
| Y7.5 | 0.07 | 0.08 | 0.06 | 0.10 | 0.08 | 0.11 | 0.14 | 1.38 | |
| Y10 | 0.14 | 0.09 | 0.07 | 0.11 | 0.07 | 0.11 | 0.14 | 1.32 | |
| Y15 | 0.08 | 0.08 | 0.07 | 0.11 | 0.09 | 0.11 | 0.14 | 1.32 | |
| Y20 | 0.10 | 0.08 | 0.07 | 0.11 | 0.07 | 0.10 | 0.15 | 1.34 | |
| Y0 | Fraction/% | - | - | 0.6 | - | 1 | - | 1.8 | 96.5 |
| Y1 | 0.1 | 0.7 | 0.2 | 0.7 | 0.1 | 0.1 | 2 | 96.1 | |
| Y2 | 0.7 | 0.9 | 0.5 | 1.7 | 0.4 | 0.7 | 6 | 89.1 | |
| Y5 | 1.5 | 0.5 | 1.3 | 1.9 | 0.2 | 1.3 | 4.8 | 88.4 | |
| Y7.5 | 0.8 | 1.4 | 3.3 | 2 | 0.9 | 3.4 | 8.8 | 79.3 | |
| Y10 | 1.6 | 1.3 | 2.7 | 2.7 | 0.3 | 1.5 | 5.1 | 84.8 | |
| Y15 | 2.5 | 4.4 | 10.2 | 6.4 | 0.9 | 3.3 | 8.7 | 63.6 | |
| Y20 | 2.9 | 4 | 8.9 | 5.5 | 0.4 | 2.3 | 7.3 | 68.7 | |
Fig. S3 Variation of relative integrated intensities (fractions) of individual phosphorescence peaks with Y doping concentration after 10 Mrad irradiation
Fig. S4 Photoluminescence excitation and emission spectra of Y20 sample (a) Excitation (λem = 595 nm) and emission (λex =399 nm) spectrum; (b) Excitation (λem = 541 nm) and emission (λex = 379 nm) spectrum; (c) Excitation (λem = 479 nm) and emission (λex = 350 nm) spectrum; (d) Emission (λex = 218 nm) spectrum
| Phosphorescence peak | Ion | 4f-4f transition | Wavelength/nm |
|---|---|---|---|
| 379 nm (3.27 eV) | Tb3+ | 5D3→7F6 | 379-381[S1] |
| 413 nm (3.00 eV) | Tb3+ | 5D3→7F5 | 414[S1] |
| 435 nm (2.85 eV) | Tb3+ | 5D3→7F4 | 435-437[S1] |
| 487 nm (2.55 eV) | Dy3+ | 4F9/2→6H15/2 | 479-488[S2] |
| 545 nm (2.27 eV) | Tb3+ | 5D4→7F5 | 541-548[S1] |
| 586 nm (2.12 eV) | Tb3+ | 5D4→7F4 | 582-589[S1] |
| 617 nm (2.01 eV) | Eu3+ | 5D0→7F2 | 609-627[S1] |
Table S1 Narrow phosphorescence peaks of Y20 sample correspond to 4f-4f transitions
| Phosphorescence peak | Ion | 4f-4f transition | Wavelength/nm |
|---|---|---|---|
| 379 nm (3.27 eV) | Tb3+ | 5D3→7F6 | 379-381[S1] |
| 413 nm (3.00 eV) | Tb3+ | 5D3→7F5 | 414[S1] |
| 435 nm (2.85 eV) | Tb3+ | 5D3→7F4 | 435-437[S1] |
| 487 nm (2.55 eV) | Dy3+ | 4F9/2→6H15/2 | 479-488[S2] |
| 545 nm (2.27 eV) | Tb3+ | 5D4→7F5 | 541-548[S1] |
| 586 nm (2.12 eV) | Tb3+ | 5D4→7F4 | 582-589[S1] |
| 617 nm (2.01 eV) | Eu3+ | 5D0→7F2 | 609-627[S1] |
| [1] | ERSHOV N N, ZAKHAROV N, RODNYI P. Spectral-kinetic study of the intrinsic-luminescence characteristics of a fluorite-type crystal. Optics and Spectroscopy, 1982, 53(1):51. |
| [2] |
CHEN J, YANG F, ZHANG L, et al. Slow scintillation suppression in yttrium doped BaF2 crystals. IEEE Transactions on Nuclear Science, 2018, 65(8):2147.
DOI URL |
| [3] | HU C, XU C, ZHANG L, et al. Improvement of scintillation performance in large size yttrium doped BaF2 crystals. 2018 IEEE Nuclear Science Symposium and Medical Imaging Conference (NSS/MIC), Sydney, 2018: 1-2. |
| [4] | CHEN J, LI X, DU Y, et al. Optical transmittance of large, high quality Y doped barium fluoride scintillation crystals. Journal of Synthetic Crystals, 2019, 48(8):1403. |
| [5] |
XU J, ZHENG J, LI X, et al. Influence of yttrium concentration on scintillation performance of heavily y-doped barium fluoride crystals. IEEE Transactions on Nuclear Science, 2025, 72(7):2000.
DOI URL |
| [6] | PEZZULLO G, BUDAGOV J, CAROSI R, et al. Progress status for the Mu2e calorimeter system. Journal of Physics: Conference Series, 2015, 587: 012047. |
| [7] | HU C, ZHANG L, ZHU R Y. Ultrafast inorganic crystals with mass production capability for future high-rate experiments. Journal of Physics: Conference Series, 2022, 1162(1):012022. |
| [8] | WANG Z, GUARDINCERRI E, RATHMAN D D, et al. Gigahertz (GHz) hard X-ray imaging using fast Scintillators. Hard X-Ray, Gamma-Ray, and Neutron Detector Physics XV, San Diego, 2013: 192-204. |
| [9] |
HU C, ZHANG L, ZHU R Y, et al. Ultrafast inorganic scintillator-based front imager for Gigahertz hard X-ray imaging. Nuclear Instruments and Methods in Physics Research Section A: Accelerators, Spectrometers, Detectors and Associated Equipment, 2019, 940: 223.
DOI URL |
| [10] | WANG H, LIU F, WANG Y, et al. Study on performance of yttrium doped BaF2. Nuclear Techniques, 2020, 43(3):21. |
| [11] |
CAFFREY A J, HEATH R L, RITTER P D, et al. Radiation Damage Studies on BAF2 and BGO Scintillator Materials. IEEE Transactions on Nuclear Science, 1986, 33(1):230.
DOI URL |
| [12] | BYRUM K, CORRODI S, OKSUZIAN Y, et al. Mu2e-II: muon to electron conversion with PIP-II. (2022-01-26)[2026-01-27]. http://arxiv.org/abs/2203.07569. |
| [13] | HU C, ZHANG L, ZHU R Y. Fast and radiation hard inorganic scintillators for future HEP experiments. Journal of Physics: Conference Series, 2022, 2374(1):012110. |
| [14] | CHEN Y, GU Y. Study on radiation damage of domestic high-Z scintillation crystals. Nuclear Electronics & Detection Technology, 1993, 13(1):12. |
| [15] |
YANG F, ZHANG L, ZHU R Y. Gamma-Ray induced radiation damage up to 340 Mrad in various scintillation crystals. IEEE Transactions on Nuclear Science, 2016, 63(2):612.
DOI URL |
| [16] | HOU Y, LIU J, YANG L, et al. Scintillation properties and irradiation damage of large size BaF2 scintillation crystals grown by Bridgman method. Journal of Synthetic Crystals, 2023, 52(4):584. |
| [17] |
WANG C, ZHANG L, HU C, et al. Radiation damage in 20-cm long LYSO:Ce and BaF2:Y crystals. IEEE Transactions on Nuclear Science, 2024, 71(9):2116.
DOI URL |
| [18] |
KOZMA P, KOZMA P. Radiation resistance of heavy scintillators to low-energy gamma-rays. Radiation Physics and Chemistry, 2004, 71(3):705.
DOI URL |
| [19] | ZHU Y, CHEN Y, SHI H, et al. Experimental study on radiation damage of domestic CsI(Tl) crystals. High Energy Physics and Nuclear Physics, 1998, 22(10):3. |
| [20] |
CHAKRABORTY P K, RAO K V. Optical absorption of BaF2 crystals irradiated with γ-rays. Journal of Materials Science, 1987, 22(2):587.
DOI URL |
| [21] | BEAUMONT J H, HAYES W. M centres in alkaline earth fluorides. Proceedings of the Royal Society of London. A. Mathematical and Physical Sciences, 1969, 309(1496):41. |
| [22] |
ATOBE K. A new absorption band in uranium doped and undoped BaF2 irradiated reactor neutrons. Journal of the Physical Society of Japan, 1979, 47(4):1377.
DOI URL |
| [23] | MA F, ZHANG Z, JIANG D, et al. Cluster structure of rare earth doped fluorite halide crystals. Journal of Synthetic Crystals, 2023, 52(7):1219. |
| [24] |
YANG F, HU C, ZHANG L, et al. UV-visible reflectance of common light reflectors and their degradation after an ionization dose up to 100 Mrad. Nuclear Instruments and Methods in Physics Research Section A: Accelerators, Spectrometers, Detectors and Associated Equipment, 2021, 992: 165043.
DOI URL |
| [25] | WOODY C L, KIERSTEAD J, LEVY P, et al. Radiation-damage in BaF2 crystals. IEEE Tran actions on Nuclear Science, 1992, 39(4):515. |
| [26] | SUN J, XIA Z, DU H. Research progress in rare-earth red long-afterglow luminescent materials. Journal of the Chinese Rare Earth Society, 2005, 23(3):257. |
| [1] | WANG Huajin, KOU Huamin, WANG Yongzhe, JIANG Dapeng, ZHANG Bo, QIAN Xiaobo, WANG Jingya, ZHU Linling, ZENG Aijun, YANG Qiuhong, SU Liangbi. Irradiation Damage of CaF2 with Different Yttrium Concentrations under 193 nm Laser [J]. Journal of Inorganic Materials, 2023, 38(2): 219-224. |
| [2] | OUYANG Qin, WANG Yanfei, XU Jian, LI Yinsheng, PEI Xueliang, MO Gaoming, LI Mian, LI Peng, ZHOU Xiaobing, GE Fangfang, ZHANG Chonghong, HE Liu, YANG Lei, HUANG Zhengren, CHAI Zhifang, ZHAN Wenlong, HUANG Qing. Research Progress of SiC Fiber Reinforced SiC Composites for Nuclear Application [J]. Journal of Inorganic Materials, 2022, 37(8): 821-840. |
| [3] | LI Feng-Rui, GU Mu, HE Hui, CHANG Li-Hua, WEN Wei-Feng, LI Ze-Ren, CHEN Liang, LIU Jin-Liang, OUYANG Xiao-Ping, LIU Xiao-Lin, LIU Bo, HUANG Shi-Ming,NI Chen. Fluorescent Decay Time and Energy Response of γ-CuI Crystal [J]. Journal of Inorganic Materials, 2017, 32(2): 163-168. |
| [4] | SHENG Yu-Bang, XING Rui-Xian, LUAN Huai-Xun, LIU Zi-Jun, LI Jin-Yan, DAI Neng-Li. Gamma Radiation Effects on the Optical Properties of Yb-doped Silicate Glasses [J]. Journal of Inorganic Materials, 2012, 27(8): 860-864. |
| [5] |
LIAO Jia-Xuan,WANG Hong-Quan,PAN Xiao-Feng,FU Xiang-Jun,ZHANG Jia,TIAN Zhong.
Surface Structures and Dielectric Properties of Yttrium-doped Barium Strontium Titanate Films by Improved Sol-Gel method [J]. Journal of Inorganic Materials, 2009, 24(2): 387-391. |
| [6] | XIAO Hai-Bin,HU Guan-Qin,XU Li. Influence of Temperature Gradient on Radiation Damage of BGO Crystals [J]. Journal of Inorganic Materials, 2003, 18(2): 470-474. |
| [7] | SHEN Ding-Zhong,REN Guo-Hao,WANG Shao-Hua,DENG Qun,YIN Zhi-Wen. Growth And Cherenkov Radiation Characteristics of PbF2 Crystals [J]. Journal of Inorganic Materials, 1999, 14(1): 12-16. |
| Viewed | ||||||
|
Full text |
|
|||||
|
Abstract |
|
|||||