Cu/Mg比对Cu/Mg-MOF-74的CO2吸附性能的影响
|
凌洁, 周安宁, 王文珍, 贾忻宇, 马梦丹
|
Effect of Cu/Mg Ratio on CO2 Adsorption Performance of Cu/Mg-MOF-74
|
LING Jie, ZHOU Anning, WANG Wenzhen, JIA Xinyu, MA Mengdan
|
|
表2 不同Cu/Mg比Cu/Mg-MOF-74的孔结构
|
Table 2 Pore structure of Cu/Mg-MOF-74 according to different Cu/Mg ratios
|
|
Parameter | 1/0 | 0.83/0.17 | 0.8/0.2 | 0.6/0.4 | 0.22/0.78 | 0.1/0.9 | 0/1 | N2 adsorption | VTotal /(cm3·g-1)a | 0.336 | 0.332 | 0.360 | 0.428 | 0.492 | 0.556 | 0.456 | VMic /(cm3·g-1)a | 0.265 | 0.257 | 0.304 | 0.362 | 0.438 | 0.520 | 0.435 | STotal /(m2·g-1)a | 1035 | 1013 | 1235 | 1562 | 1917 | 2395 | 1611 | SMic /(m2·g-1)a | 1020 | 996 | 1223 | 1533 | 1889 | 2371 | 1590 | d1 / nmb | 0.774 | 0.769 | 0.760 | 0.767 | 0.763 | 0.763 | 0.751 | CO2 adsorption | UVMic /(cm3·g-1)c | 0.143 | 0.027 | 0.0735 | 0.181 | 0.246 | 0.322 | 0.129 | USMic /(m2·g-1)c | 796.2 | 151.9 | 422.0 | 1003 | 1376 | 1800 | 714.7 | d2 /nmb | 0.612 | 0.699 | 0.681 | 0.612 | 0.555 | 0.539 | 0.578 |
|
|
|