表2 Na3Zr2Si2PO12固体电解质生坯、陶瓷片烧结参数与致密度测量参数与结果
Table 2 Sintering parameters and density measurement parameters and measurement results of Na3Zr2Si2PO12 solid electrolyte green bodies and ceramic sheet
Sample Process temp./℃ Time/h m/g rethanol/(g·cm-3) msubmerged/g rreal/(g·cm-3) rtheoretical/(g·cm-3) rrelative/%
GB - - 0.2902 0.785 0.2056 2.693 3.244 83.01
SD-GB - - 0.2880 0.785 0.2098 2.891 3.244 89.12
CS-NZSP 1250 6 0.2672 0.785 0.1938 2.858 3.244 88.10
SD-CS-NZSP 1250 6 0.2644 0.785 0.1988 3.164 3.244 97.53