第三代SiC纤维及其在核能领域的应用现状
|
王堋人,苟燕子,王浩
|
Third Generation SiC Fibers for Nuclear Applications
|
WANG Pengren,GOU Yanzi,WANG Hao
|
|
表1 三代SiC纤维的组成和力学特性[5,13-18]
|
Table 1 Compositions and mechanical properties of three generations SiC fibers[5,13-18]
|
|
| Trade mark | Tensile strength/GPa | Young’s modulus/GPa | Diameter/μm | C/Si | First generation | Nicalon 200 | 3.0 | 200 | 14 | 1.33 | Tyranno Lox-M | 3.3 | 185 | 11 | 1.38 | KD-I | >2.5 | >170 | 11.5 | 1.29 | Second generation | Hi-Nicalon | 2.8 | 270 | 12 | 1.39 | Tyranno ZE | 3.5 | 233 | 11 | 1.34 | KD-II | >2.7 | >250 | 11.5 | 1.35-1.40 | Third generation | Hi-Nicalon S | 2.6 | 340 | 12.0 | 1.05 | KD-S | 2.7 | 310 | 11.0 | 1.08 | Tyranno SA | 2.8 | 375 | 8.0&10.0 | 1.08 | KD-SA | 2.5 | 350 | 10.5 | 1.05 | Sylramic | 3.2 | 400 | 10.0 | 1.01 |
|
|
|