表1 针刺碳/碳复合材料参数
|
Table 1 Parameters of needled C/C composites
|
|
No. | ρA-fiber web/ (g·m-2) | ρA-weftless ply/ (g·m-2) | Needling depth/ mm | Needling density/ (pin·m-2) | ρpreform/ (g·cm-3) | ρC/C/ (g·cm-3) | Porosity/ % | A | 200 | 300 | 12 | 22 | 0.31 | 2.073 | 0.677 | B-1 | 140 | 340 | 12 | 12 | 0.45 | 2.052 | 0.528 | B-2 | 140 | 340 | 12 | 22 | 0.44 | 2.047 | 0.680 | B-3 | 140 | 340 | 12 | 27 | 0.44 | 2.052 | 0.681 | B-4 | 140 | 340 | 12 | 35 | 0.45 | 2.048 | 0.570 | B-5 | 140 | 340 | 15 | 12 | 0.44 | 2.042 | 0.622 | B-6 | 140 | 340 | 18 | 12 | 0.44 | 2.040 | 2.361 | B-7 | 120 | 300 | 12 | 22 | 0.46 | 2.040 | 1.643 | B-8 | 140 | 340 | 12 | 22 | 0.45 | 2.048 | 1.416 | C | 80 | 380 | 12 | 22 | 0.6 | 2.016 | 1.127 |
|
|
|